Skip to main content

Johnson Cook failure model

Submitted by solat.noruzi on

Hi

can Anyone help me to find johnson-cook failure model damage parameters(d1, d2, d3, d4) for Advanced hgih strength steels like DP and TRIP?

thanks

From http://adsabs.harvard.edu/abs/2006AIPC..845..775V

 "J-C strength
model constants for mild steel are A=217 MPa, B = 234 MPa, n = 0.643 and
C = 0.076 and for DP590 steel are A = 430 MPa, B = 824 MPa, n = 0.510
and C = 0.017".  You might try to contact the authors and see whether they have any experimental data on failure.  Then fit your own parameters.

Alternatively, look at  http://web.mit.edu/icl/AHSS_Technical_Aug_15%20_final_.pdf and use some of the data/references they have provided.

 

Mon, 03/09/2009 - 02:24 Permalink

have read the MIT proposal before but my problem is that there is no
failure parameter in papers for advanced high strength steels, and I
don't have experiment data to find them.

thanks for your attention and guides.

finding damage parameter need 3 tests(shear test, uniaxial tension test on notched and smooth specimen), so how can I get these parameter just by modeling not experiment?

is it possible or no? if it is possible with needs to less experiment test data, which tests are needed?

 

Mon, 03/09/2009 - 22:05 Permalink

Why do you need a notched tensile test?  You will find such data very hard to come by for high strain rates and high temperatures. 

Johnson-Cook damage model parameters are hard to find because they are often in the classified national lab literature.  You will have no choice but to fit your own parameters for most materials.  Even that is quite difficult because of the spread in failure strain data.

The Johnson-Cook damage model gives the plastic strain at failure as a function of the (mean stress/deviatoric stress), the plastic strain rate, and the temperature. See http://www.scribd.com/doc/6226594/em2004paper270 equation (20).  The three parameters D1, D2, D3 need tests under three known stress states.

If you want find these parameters numerically (without testing) then you'll have to do calculations based on the microstructure of the steel.  You will need fracture strengths of grain interfaces and bulk grains as a function of stress state.  If those fracture strengths are not available you'll have to go one step lower and try to compute them using molecular dynamics simulations.  These simulations will need the correct grain boundary potentials etc.  To find these potential you'll have to go down one more length scale (and most likely, time scale) and do some ab-initio calculations.

In my opinion it's easier to search for data in the literature and fit the parameters you need.

-- Biswajit 

Tue, 03/10/2009 - 02:24 Permalink