Advanced materials that can sustain extreme heat fluxes and heat loads are in increasing demand in recent years, driven by human desire to travel faster and facilitated by major nations’ recently reiterated initiatives on (manned) space exploration. A recent example is the establishment of a National Hypersonic Science Center for Materials and Structures, supported jointly by AFOSR and NASA and dedicated to the research and development of novel materials and structures that can withstand high temperature environment of > 1700 ºC for sustained period of time (for readers wish to know more about the fascinating history and current challenges specific to hypersonic vehicles, we recommend a recent article by Bertin and Cummings [1]. But here we shall focus our discussions on UHT-materials and the related thermal mechanics).
In general, increasing material operating temperature can greatly improve the performance of a variety of important mechanical and material systems such as reentry space shuttles, hypersonic vehicles, rocket nozzles, turbine blades and combustor liners, and other thermal protection systems.
The challenges in materials development for UHT applications have been fully appreciated since the Apollo era [1]. The very basic requirements are that the microscopic crystal structures should be stable and not subject to extensive oxidation. However, this has proved to be difficult to meet: most metals or metal alloys under UHT environment tend to suffer from microstructure evolution which leads to significant creep deformation and oxidation; UHT(monolithic) ceramic materials, on the other hand, can sustain UHT with much less creep deformation, but they are typically too brittle to meet structural requirements. Recent developments in diborides of zirconium (ZrB2)and of hafnium (HfB2) have demonstrated very promising oxidationresistance under UHT environments (up to 2200 ºC) [2]. Another type of promising ceramics are the polymer-derived ceramics (PDCs) which are made directly by heating Si-based polymers to about1000 ºC, during which the scission of C-H bonds evolves hydrogen leaving behind a ceramic constituted from Si, C, N and O. These ceramics show zero creep up to 1500 ºC despite being "amorphous" [3,4]. However,such materials are still very expensive to make and their strength-to-weight ratios remain too small for large scale usage. They now are used only in those most critical UHT areas such as the leading edge of high-speed aero-vehicles.
With consideration of strength-to-weight ratio, material selection favors more toward the toughed ceramic matrix composites (CMCs). In such materials, high strength, high temperature resisting fibers (C, SiC or Oxides) are embedded in (brittle) ceramic matrices (C or SiC) [5]. It has been well established that through secondary matrix cracking and interface debonding, such materials can achieve reasonable high strength at high temperature. However, due to the multiple cracking nature of such materials, careful consideration of progressive damage evolution is mandatory. A very comprehensive review on the physics and mechanics of classic CMC laminates can be found in [5] and the references therein. Note that in this paper the mechanisms of most of the failure modes are assumed to operate independently. In realty, multiple failure modes may operate in a strongly coupled manner and how to account for the coupled evolution of multiple damages (which may operate at different length and time scales) remains a challenging issue up to date. Another critical issue with CMC laminates is that they tend to delaminate under severe thermal gradients, which are inevitable under UHT environments.
Recently, an exciting new paradigm of CMCs based on the use of three-dimension fiber reinforcement that enables functionality in heat exchange, transpiration, detailed shape, and thermal strain management that significantly exceeds the prior art have been developed Two such examples are given in Figure 1 and Figure 2. Such structures can be tailored to the specific shape, stress, and thermal requirements of a structural application and therefore generally requires innovative textile methods for each realization. The current state-of-art design of such materials and structures has been given in [6], wherein the design considerations, textile processing, thermal management, thermal-mechanical stress analyses, and prototype demonstrations of several high temperature CMC components are presented as detailed case studies. It is worth pointing out that the unique design for targeted applications (i.e. non-standard design procedure) can pose potential challenges in assuring product quality and predict performance prior to investment in fabrication and testing [6]. Regard to this, high fidelity numerical models that can faithfully simulate the material response under UHT environments become extremely valuable, which have prompted increasing investment into this research area recently. The major challenges in modeling the progressive failure of UHT materials and structures include but not limited to: 1) stochastic initial imperfections due to fiber tow displacement, void allocation, and processing induced cracking/damages; 2) coupled multiple cracking evolution and their instantaneous interaction with temperature field(Figure 2 & 3); 3) transient coupling among multiple arbitrary cracking, material softening (due to HT) and material damage due to oxidation; and 4) linking and cross-talking among vastly different temporal and spatial scales that the various mechanisms operate on. Possible methods to build such high fidelity capabilities are discussed in [7].
Figure 1 3D woven CMC tube structure for UHTapplication including its textile weave (a), 3D interlacing (b), and (c) finalprototype and its multiscale features. For this panel the inside of the tubes passes liquid H2 fuel while the bottom side are exposed tocombustion environment with temperature ~ 3300 0C
Figure2 A SiC-SiC combustor liner with transipiration holes.
Figure 3 Cross-section view of initial imperfections and complex damages in a CMC, which pose significant challenges forhigh-fidelity modeling
References:
[1] Bertin, J. J. and Cummings,R. M. (2003). FiftyYears of Hypersonics: where we’ve been, where we’re going. Progressin Aerospace Science. Vol 39 (6-7): 511-536.
[2] William G. Fahrenholtz,w and Gregory E. Hilmas, et al. (2007). RefractoryDiborides of Zirconium and Hafnium. Journal of American Ceramic Society. 90(5): 1347-1364.
[3] PaoloColombo, Gabriela Mera, et al.(2010). Polymer-DerivedCeramics: 40 Years of Research and Innovation in Advanced Ceramics. Journal of the American Ceramic Society, 93(7),1805-1837.
[4] Brahmandam, S. and Raj, R. (2007). Novelcomposites constituted from hafnia and a polymer-derived ceramic as aninterface: Phase for severe ultrahigh temperature applications. Journal ofthe American Ceramic Society, Vol 90(10): 3171-3176.
[5] A. G. Evans and F. W. Zok (1994). The physics and mechanicsof fiber-reinfirced brittle matrix composites. Journal of Material Science. Vol. 29 (15): 3875-3896.
[6] D. B. Marshall and B. N. Cox (2008). IntegralTextile Ceramic Structures. Annual Review of Materials Research. Vol 38:425-443.
[7] B. N. Cox and Q. D. Yang (2006). InQuest of Tests for Structural Composites. Science. Vol 314 (5802):1102-1107.
May you list natural high temperature resisting materials?
Thanks Qingda for the interesting topic. May you please list natural high temperature resisting materials? I am thinking how mother nature solves this problem.
Re: natural high temperature resisting materials
XiaoDong,
Thanks a lot for raising this interesting question. I think nature makes ht resisting materials, such as rocks, silica, and all sorts of quartz, by subjecting them through a even higher temperature (with high pressure) process (we are talking about geo-time scale now). My understanding is that through such processes only HT resisting elements remain and the bond is mostly covalent. As a result, the monolithic form of such materials are typically very brittle and not well suited for structural purpose, especially there tensile strength is very poor.
Re: natural high temperature resisting materials
I do not think in nature there are any living creatures that can withstand the temperture as high as that mentioned by Qingda (> 1700 ºC). The documented thermal limit for metazoan life at hydrothermal vents should be considered to be above 45 °C, but less than 60 °C. It was reported that Alvinella pompejana, a vent-chimney alvinellid worm, lives under sustained temperatures of 60 °C, which could make it the Earth's most thermotolerant metazoan [1]. Recently, we characterized [2] the shell of a deep-sea hydrothermal snail (Crysomallon squamiferum) and found that its shell is composed of a sandwich structure with a relative thick organic layer embeded between two ceramic layers (greigite Fe3S4 and aragonite CaCO3). Computational studies indicated that such sequence of these three layers is benifical for the thermal resistance of the whole structure.
[1]. Cary, S. C., T. Shank, and J. Stein. 1998. Worms bask in extreme temperatures. Nature 391, 545–546.
[2]. Haimin Yao, Ming Dao, Timothy Imholt, Jamie Huang, Kevin Wheeler, Alejandro Bonilla, Subra Suresha, and Christine Ortiz, 2010. Protection mechanisms of the iron-plated armor of a deep-sea hydrothermal vent gastropod, PNAS 19, 987–992.
In reply to Re: natural high temperature resisting materials by Haimin Yao
Re: natural high temperature resisting materials
Haimin:
read yours and Cary et al paper ... fascinating stuff. I am especially interested in how the Pompeii worms can survie a temperature gradient of 60 C with maximum temperature exceeds 80 C (most creature will become edible ^_^ at such temperature environment). Do you aware any study besides yours on the thermal management of the worms? I shall look up too ...
Haimin: Thanks a lot for the
Haimin:
Thanks a lot for the interesting information on how living creatures cope with high temperature, although understandably they do not have to survive 1000+ deg-C of temperature. However, it is rather amusing to see that nature can evolve out a thermal protection system (TPS) needed by these creatures. TPS is an absolute necessity in hypersonic vehicles and the sandwich structure you mentioned is one of the major concepts now used. Such an example is also illustrated in Fig 11 of reference [6] in my introduction. I shall read the two papers you mentioned to see if we can gain more insights from omni-powerful nature mother.
Re: Mechanical Propertis of Heat Treated Nacre
Thanks Haimin and Qingda. Good points. Natural biological materials, like engineering materials, also get phase transformation/change from room temperature to high temperature. It is of interest to see the correlation between microstructure and mechanical properties. My group heated nacre and found some interesting stuff.
Z. W. Huang and X. D. Li, Nanoscale Structural and Mechanical Characterization of Heat Treated Nacre, Materials Science and Engineering C, 29 (2009) 1803-1807.
In reply to Re: Mechanical Propertis of Heat Treated Nacre by Xiaodong Li
Re: Mechanical Propertis of Heat Treated Nacre
v\:* {behavior:url(#default#VML);}
o\:* {behavior:url(#default#VML);}
p\:* {behavior:url(#default#VML);}
.shape {behavior:url(#default#VML);}
v\:textbox {display:none;}
Re: Mechanical Propertis of Heat Treated Nacre
Thanks a lot. Yes. Biopolymer also exists inside individual platelets (bricks) and contributes to the in-plane toughness of the bricks (see the paper below). The introduction of another material constituent in CMC structures is a excellent idea, mimicking nacre.
For >500 C, we did not measure the fracture toughness of nacre. I think it will be of interest to do such tests.
Li X, Huang Z (2009) Unveiling the Formation Mechanism of Pseudo-Single-Crystal Aragonite Platelets in Nacre, Phys Rev Lett, 102, 075502.
Re: Mechanical Propertis of Heat Treated Nacre
Thanks for the explanation -- very interesting. If so, the in-plane biopolymer could be in connection with the biopolymer layer between the inter plateletts, which in turn would provide extra toughening to the interface through bridging. Have you ever looked at this? The bridging effects can be significant ...
What kind of creep?
Qingda,
If I understand correctly from your article, it seems that the main problem with conventional structural materials is high temperature creep. Broadly, this could indicate mechanisms from two distinct categories: dislocation creep or diffusional flow. For materials of interest for high temperature applications (refractory alloys, high T_m ceramics), do you know which of these two kinds of creep is dominant?
MJD
In reply to What kind of creep? by demkowicz
Re: What kind of creep?
Michael,
Thanks for asking. It's mostly dislocational creep with power index of 3~5 and we are talking about the life time of several to tens of hours.
In reply to Re: What kind of creep? by Qingda Yang
Thanks!
Thanks!