Skip to main content

Abaqus

Submitted by kdevarajanmts on

 hello everyone.

 

iam devarajan.k currently pursuring M.Tech in Engineering Design in Amrita University and doing projects on hot rolling of thick plates.For FEm simulation iam using ABAQUS software. After material rolled, i want to quench that material into water or some other material. i dont know how to do this in abaqus. please guide me if any one know this. please

 

With Regards

Devarajan.K

iam devarajan.k currently pursuring M.Tech in Engineering Design in
Amrita University and doing projects on hot rolling of thick plates.For
FEm simulation iam using ABAQUS software. After material rolled, i want
to quench that material into water or some other material. i dont know
how to do this in abaqus. please guide me if any one know this. plea

Fri, 10/07/2011 - 16:11 Permalink

 

 

Hello,

you need to use FILM

see: โ€œThermal loads,โ€  Section 30.4.4 of the Abaqus Analysis User's Manual



also:

1.6.4 Quenching of an infinite plate

in the Benchmark Manual

 

------------------------------------------
Ruhr-University
Bochum
Germany

Mon, 10/10/2011 - 08:44 Permalink

i am modelling impact on composit (CFRP) sadwitched between aluminium plates in FEM using ABAQUS6.10.On submitting the job the errors-

1-ELASTIC CONSTANTS ENTERED ARE NOT PHSICALLY REASONABLE:-CHECK FOR POISSION   RATIOS.

2- ELASTIC CONSTANTS ENTERED ARE NOT PHSICALLY REASONABLE.WORK DONE BY ALL STRAIN COMPONENTS MUST BE PSITIVE.CHECK FOR POISSION RATIOS.

IF ANY ONE HAVE ANY CLU/SOLUTION PLEASE SUGGEST.THANK YOU. 

Mon, 10/10/2011 - 10:29 Permalink